Skip to content
ISO 9001 · MTC Certified · ASTM / UNS Standards
Blog

Choosing Corrosion Resistant Alloys by Environment: High Temperature, Chemical Exposure and Constant Wet Service

Choosing Corrosion Resistant Alloys by Environment: High Temperature, Chemical Exposure and Constant Wet Service

Two sets of Ni-Resist pump casings at an Arabian Gulf desalination plant corroded at the same rate in lab tests, 0.20–0.25 mm per year in brine. One set lasted 18 years. The other lasted five. Same alloy family, same plant, same water, and a 13-year gap that no corrosion-rate table would have predicted.

That’s the problem with asking “how long will this alloy last?” without describing where it’s going. Hot gas, liquid chemicals and permanent wetness each break down the protective film in a different way, so an alloy’s ranking moves when the environment moves. Hastelloy X lost about a third as much metal as Inconel 601 in a Haynes burner-rig test at 980°C, yet 601 is the alloy many furnace builders pick for clean-air muffles. Neither fact is wrong. They describe different environments.

Below we go through high-temperature, chemical and constant-wet service in turn, with the manufacturer data and failure studies behind each recommendation, and a quick-reference table at the end.

Key Takeaways

  • High temperature isn’t one environment. Oxidation, sulfidation and carburization each favor different alloys. Nickel alloys that excel in clean hot air can fail fast in sulfur-bearing gas above about 645°C.
  • In chemical service, the limits are sharp. Hastelloy C-2000 runs at 0.36 mm/y in boiling 3% hydrochloric acid and 1.61 mm/y at 3.5%. Half a percent of concentration moves it from usable to scrap.
  • “Newer” alloys solve specific gaps, not every problem. C-2000’s copper addition targets sulfuric acid; it doesn’t make the alloy better everywhere.
  • Tungsten matters as an alloying element, not a construction material. About 3.75% tungsten helps C-276 resist localized attack. Pure tungsten oxidizes in hot air.
  • Constant wetness changes the rules for steel. The FHWA advises caution with bare weathering steel when it stays wet more than 60% of the time. Weathering steel needs to dry out to form its protective patina.
  • Corrosion-resistant cast irons are niche but real. High-silicon iron (14.20–14.75% Si per ASTM A518) handles strong acids. Ni-Resist handles seawater pumps but is sensitive to microstructure.

Why Environment Comes Before Grade

Every corrosion resistant alloy depends on a protective surface film: chromium oxide, aluminum oxide, titanium oxide or, for cast irons, silica or an austenitic nickel-rich matrix. The three environments attack that film differently:

  • High-temperature gas grows, cracks and spalls the oxide scale, or replaces it with sulfides or carbides that don’t protect.
  • Aqueous chemicals dissolve the passive film when acid strength, temperature or halide level crosses a threshold.
  • Constant wetness never lets a film dry out and stabilize. It also concentrates chlorides in crevices and under deposits.

Before we quote a CRA, we ask for the peak metal temperature (upsets included), the full chemistry down to trace sulfur, carbon, chlorides and fluorides, and how much of the time the surface is wet. Those three answers usually leave one or two alloy families standing before price is even discussed. For why no alloy survives every environment, see our explainer Is Any Alloy Truly Corrosion-Proof?.

High Temperature: Which Alloys Resist High-Temperature Corrosion Best?

Above roughly 550°C, “corrosion resistance” stops meaning resistance to liquid water. It means resistance to hot gas. Three mechanisms dominate, and each favors different alloys.

Oxidation in combustion gas

Oxidation is the baseline mechanism. Chromium (and in some alloys aluminum or silicon) forms a slow-growing oxide scale. The question is how long that scale holds up when it’s heated and cooled repeatedly.

Haynes International publishes one of the clearest comparisons. It’s a burner-rig test in which samples sit in the combustion products of No. 1 and No. 2 fuel oil and are cycled below 280°C every 30 minutes. The figure reported is metal affected: surface loss plus internal attack.

Alloy980°C, 1,000 h (µm affected)1,095°C, 500 h (µm affected)
HAYNES 23089145
Hastelloy X (Alloy X)163343
RA330300343
Incoloy 800H389691 (after 400 h)
Type 310 stainless419612
Inconel 600452526
Inconel 601508>610
Type 304 / 316 stainless>504 after only 6.5 hnot tested

Source: Haynes 230 alloy datasheet, “Resistance to High-Temperature Combustion Gas Environments.”

The 304 and 316 rows are the ones to show anyone proposing ordinary stainless for a burner component: both passed 504 µm of attack in six and a half hours, a level the nickel alloys took 1,000 hours to approach. Among the grades we stock, Alloy X comes out best, with roughly a third of the attack seen on 600 or 601 at 980°C. (Its 8–10% molybdenum and 0.2–1.0% tungsten are there mainly for high-temperature strength.)

The 601 result surprises people. 601 is usually preferred over 600 for furnace muffles and baskets in clean air, because its 1.4% aluminum forms a more adherent scale under thermal cycling. We explain that in Inconel 600 vs 601. In this fuel-oil burner rig, where the scale is cracked by a thermal cycle every 30 minutes and exposed to combustion products, 601 fell behind. Both observations hold; they come from different environments.

Sulfidation: the hidden limit for nickel alloys

When the gas contains sulfur (H₂S, SO₂, or sulfur-bearing fuel ash), nickel becomes a liability. Brian Gleeson’s review in Materials Research (2004) explains why:

  • Nickel and nickel sulfide form a low-melting Ni–Ni₃S₂ eutectic at 645°C. Once liquid sulfide forms at the metal surface, attack accelerates sharply.
  • Sulfidation rates of the major alloying metals are typically 10⁴ to 10⁶ times higher than their oxidation rates.
  • For highly sulfidizing environments, the practical long-term service ceiling for metallic materials is about 600–650°C.
  • Chromium helps less against sulfidation than against oxidation. Cobalt and silicon help more. Gleeson credits the cobalt and silicon in HAYNES HR-160 for its sulfidation resistance.

If your gas carries sulfur and the metal runs above roughly 600°C, don’t start from a standard high-nickel alloy. Cobalt- or silicon-modified grades are the better candidates, and oxidation ratings tell you little here. Ask for sulfidation test data in a gas close to yours.

Carburization and metal dusting

In carbon-rich gas (syngas, reformer streams, ethylene cracking), carbon diffuses into the alloy and ties up chromium as carbides. A 2012 study in the Journal of the Southern African Institute of Mining and Metallurgy describes metal dusting as attack that occurs at 400–800°C when carbon activity exceeds 1. Steels and nickel alloys literally disintegrate into a mixture of metal particles and coke, usually as pits. The mechanism: chromium carbide precipitation depletes chromium until the protective chromia scale can’t be maintained.

In that study’s 650°C exposure, Alloy 602CA (high Cr plus Al) resisted metal dusting better than Alloy 800, which accumulated coke as exposure ran from 96 to 336 hours. Alloys combining high chromium with aluminum hold up best. 800H and 800HT remain the workhorses for carburizing furnace tubes because of their creep strength. We cover the grade differences in Incoloy 800 vs 800H vs 800HT.

Chemical Exposure: Concentration and Temperature Thresholds

In liquid chemical service the mechanism is different. The passive film dissolves once acid strength or temperature crosses a threshold, and the threshold is often sharp.

Haynes’s data for Hastelloy C-2000 in hydrochloric acid shows how sharp:

HCl concentration93°C (mm/y)Boiling (mm/y)
2%<0.010.09
3%0.020.36
3.5%0.651.61
4%1.242.15

Look at the 93°C column. Going from 3% to 3.5% HCl multiplies the rate by more than 30. “C-2000 is good in dilute HCl” is true at 3.0% and false at 3.5%, which is why we want the highest acid concentration the equipment will ever see, not the average, and why we check against the iso-corrosion curve instead of a one-word rating.

Chemical process plant structures lit at night
Chemical process plant structures lit at night

What newer alloys protect against, and what they don’t

“New alloy” usually means one designed to close a specific gap left by older grades. C-2000 is a good example. Haynes describes it as “unique among the versatile nickel-chromium-molybdenum materials in having a deliberate copper addition.” Its 1.6% copper greatly improves resistance to sulfuric acid, and its 23% chromium handles oxidizing contaminants such as ferric ions and dissolved oxygen. Haynes’s comparative plots show C-2000 ahead of C-22, C-276 and 625 in hydrochloric acid up to 10% and sulfuric acid up to 80%.

What the copper doesn’t do:

  • It doesn’t move the HCl threshold shown above very far. Above a few percent HCl at high temperature, nickel-molybdenum alloys such as Hastelloy B-3 or B-2 remain the specialists, provided no oxidizers are present.
  • It doesn’t change high-temperature behavior. C-2000 is an aqueous-corrosion alloy, not a furnace alloy.
  • It doesn’t remove the need to check welds and crevices. Like all Ni-Cr-Mo alloys, it resists chloride stress corrosion cracking far better than austenitic stainless steels, but crevice performance depends on the actual geometry and chemistry.

Mixed sulfuric acid with oxidizing contaminants is exactly the stream C-2000 was designed for. Pure hot hydrochloric acid isn’t, and paying the premium there buys little.

Can tungsten resist corrosion?

Tungsten shows up in corrosion conversations in two very different ways.

As an alloying element, it’s valuable. Our Hastelloy C-276 typically contains about 3.75% tungsten alongside 16% molybdenum and 15.5% chromium. Together with molybdenum, it contributes to the alloy’s resistance to pitting and crevice corrosion in reducing and chloride conditions. Alloy X carries 0.2–1.0% tungsten, mainly for high-temperature strength.

As a pure metal, tungsten is rarely a corrosion-resistant construction material. It doesn’t rust the way iron does and is resistant to many acids at room temperature. But it oxidizes readily in air once heated. Researchers studying tungsten for fusion reactors, where it may be exposed to air during accidents, study how its oxide scale grows at 400°C (Fulton & Lunev, 2019). It’s also brittle at room temperature and very dense. Hot tungsten is therefore normally used in vacuum, inert gas or hydrogen, and corrosion-resistant equipment relies on tungsten-bearing nickel alloys instead.

Constant Wet Service: Is There a Steel for Continuous Exposure?

Continuous wetness splits into two very different cases.

Freshwater and humid atmospheres: the weathering-steel trap

Weathering steel (Corten-type) is often proposed as “the steel that doesn’t need painting.” It works by forming a dense, adherent rust patina, but only if the surface can dry. FHWA Technical Advisory 5140.22 states: “If the yearly average time of wetness exceeds 60 percent, caution should be used in the use of bare weathering steel.” It also advises against bare weathering steel where chloride deposition exceeds 0.1 mg/100 cm² per day, and in tunnel-like crossings with heavy deicing salt. Even over water, it calls for clearances of at least 10 ft over stagnant water and 8 ft over running water.

For parts that stay wet most of the time, then, look elsewhere:

  • Coated or galvanized carbon steel, with a coating designed for immersion and a maintenance plan.
  • Stainless steel, matched to the chloride level. Grade 316 is common in freshwater systems; higher-PREN grades are needed as chlorides rise. Our guide to pitting corrosion and PREN shows how to match PREN to chloride and temperature.
  • Copper-nickel or titanium where water quality is poor or uncertain.
Coastal industrial port facility exposed to seawater and salt air
Coastal industrial port facility exposed to seawater and salt air

Seawater: titanium, copper-nickel, and velocity

For continuous seawater immersion, titanium and copper-nickel are the reference materials, and velocity separates them. TIMET’s corrosion manual reports:

Location and flowDurationCP titanium (mm/y)70/30 copper-nickel* (mm/y)
Wrightsville Beach, 0.6–1.3 m/s6 months0.00010.022
Brixham, 9.8 m/s12 months<0.00250.3

High-iron, high-manganese 70/30 grade. In the Brixham test, the aluminum brass sample perforated.

At normal flow, 70/30 copper-nickel corrodes at about 0.02 mm/y, which is entirely acceptable for condenser and piping service. At Brixham’s 9.8 m/s, its rate was more than ten times higher, while titanium barely registered. TIMET also reports titanium tubing that spent 16 years in a polluted-seawater condenser with only slight discoloration. We compare the copper-nickel grades in C70600 vs C71500.

Whether a steel can take continuous exposure depends on which water. In fresh water, a correctly chosen stainless or a properly coated carbon steel can; bare weathering steel can’t. In seawater, ordinary stainless steels pit and crevice-corrode. Durable choices are super-austenitic or super-duplex stainless steels, copper-nickel at moderate velocity, and titanium where velocity or pollution is high.

How to Choose a Corrosion-Resistant Cast Iron

Cast iron comes up when a component has to be cast in a complex shape (pump casings, valve bodies, anodes) and a wrought alloy would be too expensive. Two families matter.

High-silicon cast iron (ASTM A518). The current edition is A518/A518M-99(2026). It specifies 14.20–14.75% silicon for all three grades, which forms a silica-rich film in strong acids. ASTM describes all three grades as “suited for application in severe corrosive environments.” Grade 2 is particularly suited to strong chloride environments, and Grade 3 is recommended for impressed-current anodes. The trade-off is mechanical: high-silicon iron is very hard and brittle, difficult to machine, and intolerant of thermal or mechanical shock.

Austenitic Ni-Resist cast irons (ASTM A436 flake graphite, A439 ductile). Enough nickel is added to give an austenitic matrix, which improves resistance to salt water. A439 Type D2 is a common choice for seawater and brine pump casings.

The best illustration of Ni-Resist’s real-world behavior is a failure study by Alzafin and co-authors in Engineering Failure Analysis (2007). It covers brine pump casings at an Arabian Gulf desalination plant. Two pump makes in the same service lasted 18 years and 5 years. Electrochemical tests showed similar corrosion rates of 0.20–0.25 mm/y for both irons in brine at room temperature. The authors instead found differences in microstructure, tensile strength and hardness. With cast corrosion-resistant irons, casting quality can outweigh the grade on the drawing. A chemical analysis alone won’t catch the difference; microstructure and hardness reports might.

We don’t produce cast irons, weathering steel or tungsten products. We include them because they’re the benchmark many of our customers start from, and the comparison is only useful with their limits in view.

Environment-to-Alloy Quick Reference

EnvironmentMain mechanismStart withAvoid / check
Clean hot air or combustion gas, 800–1,100°COxidation, scale spallingAlloy X, Inconel 601304/316 stainless; check cyclic vs steady service
Sulfur-bearing gas, >600°CSulfidationCo- or Si-modified alloys, with sulfidation test dataStandard high-Ni alloys (Ni–Ni₃S₂ eutectic, 645°C)
Carbon-rich gas, 400–800°CCarburization, metal dustingIncoloy 800H/800HT for creep; high Cr + Al alloys for dustingLow-Cr steels
Mixed sulfuric acid with oxidizersPassive film breakdownHastelloy C-2000, C-276Exceeding the iso-corrosion line in upsets
Hot hydrochloric acid, no oxidizersReducing acid attackHastelloy B-3 / B-2Ferric or cupric ions
Humid atmosphere or fresh water, mostly wetUniform and pitting corrosionCoated carbon steel, stainless matched to chlorideBare weathering steel (wet >60% of the time)
Seawater, normal velocityPitting, crevice, foulingCopper-nickel, super-austenitic stainless, titanium304/316 in crevices
Seawater, high velocity or pollutedErosion-corrosionTitaniumCopper alloys above design velocity
Strong acid, cast shape neededAcid attackHigh-silicon iron (ASTM A518)Thermal or mechanical shock
Seawater or brine pumps, castCorrosion plus SCCNi-Resist A439 D2 with microstructure controlUnverified castings

Frequently Asked Questions

Which alloys resist high-temperature corrosion best?
It depends on the gas. In Haynes’s cyclic combustion-gas test at 980°C, HAYNES 230 and Hastelloy X showed the least attack (89 and 163 µm after 1,000 hours). Sulfur-bearing gas above about 600°C favors cobalt- or silicon-modified alloys over standard high-nickel grades. Carbon-rich gas calls for alloys combining high chromium with aluminum.

Is there a steel that can withstand constant water exposure?
Yes, but not bare weathering steel, which the FHWA cautions against when surfaces are wet more than 60% of the time. Stainless steel matched to the chloride level works in fresh water. Seawater needs super-austenitic or super-duplex stainless, copper-nickel or titanium.

How do I choose a corrosion-resistant cast iron?
Use high-silicon iron (ASTM A518, 14.20–14.75% Si) for strong acids where a hard, brittle casting is acceptable. Use austenitic Ni-Resist (ASTM A436 or A439, such as D2) for seawater and brine pumps, and require microstructure and hardness checks.

Can tungsten resist corrosion?
Pure tungsten resists many acids at room temperature but oxidizes in hot air, so it’s used in vacuum or protective atmospheres. In corrosion service, tungsten earns its place as an alloying element, as in C-276 at about 3.75%.

Are newer alloys always better than older ones?
No. Each newer alloy targets a specific gap. Hastelloy C-2000’s copper addition improves sulfuric acid resistance and it outperforms C-276 up to 10% HCl. In hotter, stronger hydrochloric acid, nickel-molybdenum alloys like B-3 remain the better choice.

Send Us the Environment, Not Just the Grade

Many inquiries we receive name a grade and a size and nothing else. Usually that’s fine. Sometimes the grade was carried over from an older project with different conditions, and we only find out after asking about temperature and chemistry. Include the operating environment with the inquiry and we’ll tell you if the grade fits, suggest an alternative if it doesn’t, and supply the material with an EN 10204 3.1 certificate. Contact our team with your service conditions.

References

  1. Haynes International. HAYNES 230 alloy datasheet, “Resistance to High-Temperature Combustion Gas Environments.” https://haynesintl.com/datasheet/haynes-230-alloy/
  2. Gleeson, B. “Alloy degradation under oxidizing-sulfidizing conditions at elevated temperatures.” Materials Research 7(1), 2004. https://doi.org/10.1590/S1516-14392004000100010
  3. Haynes International. HASTELLOY C-2000 alloy technical bulletin. https://haynesintl.com/wp-content/uploads/2023/06/c-2000.pdf
  4. U.S. Federal Highway Administration. Technical Advisory T 5140.22, Uncoated Weathering Steel in Structures (1989). https://www.fhwa.dot.gov/bridge/t514022.cfm
  5. Alzafin, Y.A., Mourad, A.H.I., Abou Zour, M., Abuzeid, O.A. “A study on the failure of pump casings made of ductile Ni-resist cast irons used in desalination plants.” Engineering Failure Analysis 14(7), 2007, pp. 1294–1300. https://research.uaeu.ac.ae/en/publications/a-study-on-the-failure-of-pump-casings-made-of-ductile-ni-resist-/

← Back to Blog Get a Quote →
From the Blog

Latest Articles

All Articles →
1