An alloy that survives the process fluid can still fail the job. It might be too weak for the load, gall the first time a valve stem turns, crack when a cold pipe takes a knock, refuse to forge into the shape you need, or eat the aluminum part bolted to it. So when we help a buyer specify a corrosion-resistant alloy, corrosion is only the first of five questions. The other four are strength, wear and galling, impact toughness, and how the part will be formed and joined. The short answers: strength varies by a factor of two or more inside the same alloy family, so the condition matters as much as the grade. Hardness is a poor predictor of galling. Austenitic alloys keep their toughness at cryogenic temperatures where ferritic steels turn brittle. Nickel alloys, titanium, nickel aluminum bronze and some nitrogen-strengthened stainless steels all forge well enough for critical parts. And aluminum should never touch steel in a wet joint without isolation or a bonded transition piece.
The numbers below come mostly from producers’ own bulletins (AK Steel, Special Metals), the Nickel Institute, TWI and the minimums on our product pages, since adjectives like “high strength” or “good wear resistance” on a quote don’t help anyone size a part. Our article on why chromium, nickel and oxide films make alloys corrosion resistant covers the corrosion side.
Key Takeaways
- Check the condition, not just the grade. On our own product specifications, minimum tensile strength runs from 690 MPa for nickel aluminum bronze C63000 and Hastelloy C-276 to 1,240 MPa for aged Inconel 718. Titanium alloys deliver the highest strength per unit weight.
- Galling resistance doesn’t follow hardness. In unlubricated button-and-block tests, Type 304 and 316 against themselves galled at just 2 ksi (14 MPa), and hardened 440C at 560 HB galled at 11 ksi (76 MPa). Nitronic 60 against itself had not galled at 50 ksi (345 MPa).
- Strength and toughness pull against each other. Annealed 304 absorbs 209 J in a Charpy test at room temperature and still 118 J at −195.5 °C. Aged Inconel 718, at roughly 1.3 GPa, absorbs about 23 to 34 J.
Strength: The Same Family Can Differ by a Factor of Two
“Titanium” or “Inconel” on a drawing tells you very little about strength. The grade and the heat-treatment condition decide it. The table below uses the minimums published on our own product pages, along with density, because many of the buyers we work with are trading strength against weight as much as against cost.
| Alloy (condition as listed) | Min. tensile strength | Min. yield strength | Density | Tensile ÷ density* |
|---|---|---|---|---|
| Ti-5553 (STA) | 1,200 MPa | 1,100 MPa | 4.65 g/cm³ | 258 |
| Ti-17 (beta processed, STA) | 1,100 MPa | 1,000 MPa | 4.65 g/cm³ | 237 |
| Titanium Grade 5, Ti-6Al-4V (annealed) | 895 MPa | 828 MPa | 4.43 g/cm³ | 202 |
| Inconel 718 (solution annealed and aged) | 1,240 MPa | 1,035 MPa | 8.19 g/cm³ | 151 |
| Monel K-500 (aged) | 965 MPa | 690 MPa | 8.44 g/cm³ | 114 |
| Nickel aluminum bronze C63000 (hot rolled / HR50) | 690 MPa | 345 MPa | 7.58 g/cm³ | 91 |
| Hastelloy C-276 (annealed) | 690 MPa | 283 MPa | 8.89 g/cm³ | 78 |
*Our calculation, in MPa per g/cm³, from the minimum tensile strength and density on each product page.
Two patterns come out of that table. The strongest nickel alloys, such as 718 and K-500, get their strength from age hardening, a precipitation treatment applied after forming. A part bought in the annealed condition, or welded and not re-aged, won’t have those numbers. Second, the alloys chosen purely for corrosion resistance, such as C-276, have modest yield strength in the annealed condition. When a corrosive service also carries a structural load, it is common to end up with two alloys, a high-strength one for the shaft or fastener and a corrosion-first one for the wetted shell. Our comparisons of Inconel 625 vs 718 and Monel K-500 vs Monel 400 cover where each pair splits.
High strength plus biocompatibility
When the question is a metal that is both strong and biocompatible, the established answers are titanium alloys and cobalt-chromium-molybdenum. Ti-6Al-4V ELI, the extra-low-interstitial version of Grade 5 (UNS R56401), is covered for surgical implants by ASTM F136, which sets chemical, mechanical and metallurgical requirements for wrought annealed material in forms from strip to forging bar. Co-28Cr-6Mo castings for implants fall under ASTM F75, revised in May 2023. The lower interstitial content of the ELI grade trades a little strength for better ductility and fracture toughness.
What matters for a buyer is that implant use is a separate regulatory track. Standard Grade 5 meeting ASTM B348 or AMS 4911 is the same alloy family, but it is not certified to F136, and a medical device maker will need the implant specification, its current edition and full traceability. For industrial parts that only need strength, low weight and corrosion resistance together, Grade 5 or a near-beta alloy such as Ti-5553 is usually the answer.
Wear and Galling: Hardness Is a Weak Predictor
Wear covers several different failure modes, and they don’t share a single best alloy. Abrasion, where hard particles cut the surface, generally rewards hardness and hard carbides. Galling, where two metal surfaces cold-weld and tear under sliding load, is the problem that ruins valve stems, threaded fasteners and pump wear rings, and it behaves differently. Cavitation erosion, from collapsing vapor bubbles in pumps and propellers, is a third case.
Galling is where the data surprise people. AK Steel’s Nitronic 60 bulletin, distributed by HPAlloy, ranks alloys with an unlubricated button-and-block test. It reports the stress at which galling begins:
| Couple (same alloy against itself unless noted) | Threshold galling stress |
|---|---|
| Type 304 vs 304 (annealed) | 2 ksi (14 MPa) |
| Type 316 vs 316 (annealed) | 2 ksi (14 MPa) |
| Type 440C vs 440C (hardened, 560 HB) | 11 ksi (76 MPa) |
| Nitronic 60 vs Type 316 | 38 ksi (262 MPa) |
| Nitronic 60 vs Nitronic 60 (205 HB) | 50+ ksi (345 MPa), did not gall |
Source: Nitronic 60 product data bulletin, Table 1.
Hardened 440C is more than twice as hard as Nitronic 60, yet it galls at a fraction of the load. Nitronic 60’s resistance comes from its chemistry, roughly 17% chromium, 8% nickel, 8% manganese, 4% silicon and added nitrogen, rather than from hardness. The same bulletin reports better chloride pitting resistance than 316 in ferric chloride tests, and cavitation erosion resistance approaching the cobalt-base alloys. That combination is why it is used for valve stems, fasteners, pins and pump wear rings in corrosive service.
Cobalt-chromium alloys such as Stellite 6 remain the reference material for severe wear. They are cobalt-base, and Applus+ Laboratories’ materials portal lists Stellite hardness at HB 370 to 480, retained at high temperature. They are usually applied as castings or weld overlays on seats and trim. Nickel aluminum bronze is the other common answer in seawater. Our C63000 combines a self-repairing alumina-rich film with good anti-galling, erosion and cavitation behavior, which is why it is specified for pump shafts, impellers, bushings and bearings. Monel K-500 is also noted for good galling resistance alongside its seawater performance.
So on a drawing for a sliding or threaded part, we’d rather see both materials named than one. Two pieces of the same austenitic stainless steel sliding against each other is the classic galling setup, and swapping one side to a different alloy family often fixes it without touching the other.
Impact Toughness: Where Strength and Toughness Pull Apart
There’s no single “most impact-resistant metal,” because toughness depends heavily on crystal structure and temperature. The Nickel Institute explains the key split. As temperature falls, the ferritic structure becomes progressively more brittle, so ferritic stainless steels are not suitable for cryogenic service. Common austenitic stainless steels retain good toughness even down to liquid helium temperatures. Nickel is what stabilizes that austenitic structure, and it also lowers the ductile-to-brittle transition temperature in steels that remain ferritic.
Charpy V-notch data published by Total Materia shows how well austenitic grades hold up:
| Grade | 27 °C | −195.5 °C | −254 °C |
|---|---|---|---|
| 304 | 209 J | 118 J | 122 J |
| 304L | 160 J | 91 J | 91 J |
| 310 | 192.5 J | 121 J | 117 J |
| 347 | 163 J | 89 J | 77 J |
Toughness drops between room temperature and liquid nitrogen temperature, then levels off. There is no cliff.
High strength comes at a cost in toughness. Special Metals lists Inconel 718 for service from −253 °C to 704 °C, including cryogenic tankage and liquid-fueled rocket components, so it is certainly not brittle in the cold. But its room-temperature Charpy values for hot-finished, aged products are 17 to 25 ft·lb (about 23 to 34 J) at tensile strengths around 194 to 209 ksi (1.34 to 1.44 GPa). That is a fraction of annealed 304’s 209 J. For a part that sees shock loading, such as a valve body in a line that can water-hammer, a lower-strength austenitic alloy with large toughness reserve can be the safer choice than the strongest grade on the list.
If impact matters, ask for Charpy results at the minimum design temperature on the mill test certificate, rather than relying on room-temperature tensile data. Our guide to reading a CRA alloy datasheet explains where those numbers appear.
Forging a Corrosion-Resistant Part Without Stainless Steel
Stainless steel isn’t the only corrosion-resistant metal that can be forged. Most of the families we supply are available as forging stock or finished forgings:
- Nickel alloys. Inconel 718 and Monel K-500 are both supplied as custom forgings, and Special Metals lists 718 for rings and casings in aircraft and land-based gas turbines.
- Titanium. Ti-17 (AMS 4921) was developed for aircraft engine fan and compressor discs, and Ti-5553 (AMS 4907/4926) for landing gear and other heavy structural forgings. Both have deep hardenability, so thick sections reach uniform properties. Grade 5 is also forged.
- Nickel aluminum bronze. C63000 is supplied as forgings and rings as well as bar and plate.
- Nitrogen-strengthened stainless. Nitronic 60 is available as forging billets and is covered by AMS 5848 for bars and forgings.
Forging these alloys is harder than forging carbon steel, and the forge shop’s experience matters. Special Metals’ data for Inconel 718 shows why. At the same hot-working temperatures, it needs roughly three to four times the roll-gap pressure of 1020 mild steel at a 20% reduction (63.3 ksi against 22.4 ksi at the cooler end of the range). The material must be reheated when any part of it drops below 1650 °F (899 °C), and final reductions of at least 20% for open-die work and 10% for closed-die work are needed to avoid a duplex grain structure. Parts are generally air-cooled rather than water-quenched. A forging supplier who can’t describe how they control reheat temperature and final reduction is a risk on these alloys.
Aluminum Against Steel: Joining Without Galvanic Corrosion
Aluminum and steel can’t be fusion-welded directly. TWI explains that in the molten state they react to form brittle intermetallic phases, and each metal is virtually insoluble in the other. Galvanic corrosion is the second problem. In a wet joint, TWI notes, the aluminum is the side that corrodes, so it needs to be insulated from the steel.
That leaves four practical routes:
- Bimetallic transition inserts. A pre-bonded strip of steel and aluminum lets each side be welded to its own metal. The Triplate product, for example, has a steel base, a pure aluminum interlayer and a marine-grade aluminum top layer, bonded by vacuum explosion welding. Its booklet warns against preheating and states that the aluminum/steel interface must not exceed 315 °C during welding. Shipbuilders adopted these joints because riveted and bolted aluminum-steel joints corroded within a few years, helped by seawater drawn into the joint as the two metals expanded and contracted at very different rates.
- Friction welding. Because the metals never melt, friction welds stay cooler and form less intermetallic.
- Brazing. Laser brazing is used in some thin-section applications.
- Mechanical fastening with isolation. This is the most common commercial method. It depends on non-conductive washers, sleeves and gaskets, sealing against water traps, and the right fastener material.
The fastener choice follows the area-ratio rule. Stainless or other noble fasteners in a large aluminum part are a small cathode against a large anode, which is usually tolerable. Aluminum fasteners in a steel or stainless structure are the reverse and fail quickly. We cover the full hierarchy in our galvanic corrosion prevention guide, the potentials in our galvanic index chart for CRA alloys, isolation kit materials in our galvanic cell isolation guide, and CRA-to-carbon-steel transitions in our guide to welding dissimilar metals.
Writing It Into the Purchase Order
Most of the problems we see after delivery trace back to a purchase order that named a grade and nothing else. The strength, galling, toughness and joining questions above turn into a short list of things to write down. State the heat-treatment condition and the minimum tensile and yield strength, not just the alloy name. For sliding or threaded parts, name the mating material and whether the couple has been checked for galling. For anything that can see shock or low temperatures, give the minimum design temperature and the Charpy requirement at that temperature. If the part is forged, say so, and ask how the forge controls reheat and final reduction. If it touches another metal, list that metal and the planned isolation or transition method.
We supply nickel alloys, titanium, nickel aluminum bronze and copper-nickel in bar, plate, pipe and forging stock with EN 10204 3.1 mill test certificates. If you send us the load, the mating parts, the temperature range and the process fluid, our team can shortlist grades and conditions that meet all five requirements, not just the corrosion one. Contact us here.
Frequently Asked Questions
Which alloy is the most wear-resistant?
It depends on the type of wear. For abrasion and severe sliding wear, cobalt-base alloys such as Stellite 6 (HB 370 to 480 for the family) are the usual benchmark. For galling between parts that slide against each other, Nitronic 60 resists far better than harder steels; in AK Steel’s tests it had not galled against itself at 50 ksi, while hardened 440C galled at 11 ksi. In seawater with cavitation, nickel aluminum bronze is a common choice.
Is there one metal with the best impact resistance?
At low temperatures, annealed austenitic alloys are hard to beat because they don’t have a ductile-to-brittle transition. Type 304 still absorbs 118 J in a Charpy test at −195.5 °C. High-strength aged alloys like Inconel 718 trade much of that toughness for strength, so “best” depends on whether the part is loaded statically or by shock.
What material should I use for a practical sword that won’t rust?
This is outside our usual industrial scope, but the metallurgy is the same trade-off this article describes. Corrosion-resistant alloys such as Hastelloy and titanium are poor blade materials because they can’t be hardened to hold an edge. The usual answer is a hardenable martensitic stainless steel. Type 440C, for example, reaches about 560 HB when hardened, but it gives up some toughness and some corrosion resistance compared with austenitic grades. A blade that must take hard impacts is a compromise between edge, toughness and rust resistance, and some care against rust is still needed.
References
- HPAlloy / AK Steel, NITRONIC 60 Stainless Steel Bar and Wire, Product Data Bulletin (galling Table 1, composition, corrosion, cavitation). https://hpalloys.com/docs/hpalloy_n60book.pdf
- Nickel Institute, The Nickel Advantage: Nickel in Stainless Steel, December 2008 (toughness, DBTT). https://www.centroinox.it/sites/default/files/monografia_pdf/nickel_in_stainless_steel.pdf
- Total Materia, “Stainless Steels for Cryogenic Applications” (Charpy Table 2). https://www.totalmateria.com/en-us/articles/stainless-steels-for-cryogenic-applications
- Special Metals, INCONEL alloy 718 technical bulletin (service range, impact, hot working, roll-gap pressure). https://www.specialmetals.com/documents/technical-bulletins/inconel/inconel-alloy-718.pdf
- TWI, “Can aluminium be welded to steel?” FAQ. https://www.twi-global.com/technical-knowledge/faqs/aluminium-welding/aluminium-to-steel
- Triplate technical booklet, explosively bonded aluminium-to-steel transition joint (Aalco). https://www.aalco.co.uk/literature/files/triplate.pdf
- ASTM F136, Standard Specification for Wrought Titanium-6Aluminum-4Vanadium ELI Alloy for Surgical Implant Applications (scope via SIS listing). https://www.sis.se/en/produkter/external-categories/medical-devices-and-services-astm-vol-13/medical-and-surgical-materials-and-devices-i-e667–f2477-astm-vol-1301/astmf13613
- ASTM F75-23, Cobalt-28 Chromium-6 Molybdenum Alloy Castings and Casting Alloy for Surgical Implants. https://www.austrian-standards.at/en/shop/astm-f-75-2023-05-01~p2665595
- Applus+ Laboratories Materials Portal, “Stellite 6” datasheet. https://www.appluslaboratories.com/materials-portal/datasheet/stellite-6/-280672700
- craalloy.com product specifications: Ti-5553, Ti-17, Titanium Grade 5, Inconel 718, Monel K-500, Nickel Aluminum Bronze C63000, Hastelloy C-276 (accessed October 2026).